Wear-Generated Polymer Particles From Provisional Full-Arch Implant Prostheses: A Laboratory Protocol for Particle Generation, Characterization, and Assessment of Cellular Response
- Paper type
- Laboratory research protocol with conceptual exposure framework
- Status
- Original Work · Working Paper
Contents
Abstract
Background. Immediate full-arch implant treatment places a polymer prosthesis in function for months while implants integrate and soft tissue heals. These prostheses are made of polymethyl methacrylate or of milled or printed resins, and they wear and fracture. Wear studies report volume loss and roughness. They do not report what becomes of the lost material. In orthopedics, polymer particles in a phagocytosable size range activate macrophages and contribute to bone resorption around joint replacements. In dentistry, grinding dust from prosthetic resins is cytotoxic to macrophages in vitro, and one study detected release of microplastic particles from dentures into artificial saliva during soaking and cleaning. The searches run for this manuscript found no study that characterized particles generated by functional wear of provisional implant prostheses or that examined the response of oral cells to them.
Objective. To specify a laboratory protocol that generates wear particles from provisional prosthesis materials under controlled conditions, characterizes their number, size, shape, and composition, and measures the response of relevant cells at doses related to estimated exposure.
Framework. An exposure chain links wear volume to particle number and surface area, to the fraction retained near tissue, and to local dose. Each link is identified as established, supported in vitro, or hypothetical.
Proposed methods. Chewing simulation, brushing, and chairside adjustment of conventional, milled, and printed materials in a closed, contamination-controlled system; isolation by cascade filtration; sizing by microscopy and light-scattering methods; chemical identification by vibrational spectroscopy and pyrolysis mass spectrometry; exposure of macrophages, gingival fibroblasts, keratinocytes, and osteoblasts to endotoxin-tested particles; an exploratory study of wear on retrieved prostheses.
Central hypothesis. Materials and manufacturing routes that differ little in wear volume differ substantially in the number and size of particles they shed, and the particle fraction between 0.3 and 10 micrometers governs macrophage response.
Conclusions. Arithmetic on published wear volumes shows that particle number is indeterminate over nine orders of magnitude without a size distribution. No clinical effect of such particles has been shown, and none is claimed.
Keywords: interim prosthesis; polymethyl methacrylate; three-dimensional printed resin; wear particles; microplastics; macrophage; peri-implant tissue; exposure assessment
1. Introduction
In immediate full-arch rehabilitation, a fixed provisional prosthesis is connected to the implants on the day of surgery or shortly afterward and remains in function until the definitive prosthesis is delivered. The provisional is a polymer structure. It may be a converted denture of polymethyl methacrylate (PMMA), a prosthesis milled from an industrially polymerized PMMA blank, or one printed from a photopolymer resin [1, 2]. It is thinner and weaker than the definitive restoration and is expected to show wear. In a practice-based cohort of 17 milled PMMA full-arch interim prostheses followed for a year, survival probability at 12 months was 76% and complete fracture occurred in 17.6% [3]. Technical complications remain frequent after definitive restoration as well, with chipping or fracture of veneering material the most common prosthesis-related complication of fixed complete prostheses [4].
Wear and fracture mean loss of material, and the material goes somewhere. Most of it is presumably swallowed. Some may lodge beneath the prosthesis, on the healing mucosa, or in the peri-implant sulcus, at a time when surgical wounds are closing and implants are integrating. Whether this matters is unknown. There are two reasons to ask.
The first is the orthopedic precedent. Wear particles from polyethylene bearing surfaces and from PMMA bone cement accumulate in periprosthetic tissue, are phagocytosed by macrophages, and provoke release of cytokines that drive bone resorption [5–7]. The response depends strongly on particle size, with particles of roughly 0.3 to 10 micrometers the most active in vitro [8]. The second is the wider concern about microplastics and nanoplastics. Plastic particles have been identified in human blood, where PMMA was among the polymers detected [9], in placenta [10], and in carotid atheroma, where their presence was associated with cardiovascular events during follow-up [11]. The sources of these particles are not known, and nothing in those studies implicates dental materials. Reviews of microplastics in dentistry nonetheless identify resin-based materials as a plausible source and note that exposure data are limited and inconsistent [12, 13].
The present manuscript does not argue that provisional prostheses harm patients. It observes that a basic descriptive question has not been answered: what particles does a provisional full-arch prosthesis shed, in what numbers and sizes, and do oral cells respond to them at realistic doses? It then specifies a laboratory protocol to answer that question, and it separates at each step what is established from what is conjecture.
2. Background and Current Scientific Evidence
Provisional materials and their wear
Provisional materials fall into three groups by manufacturing route: conventional auto- or heat-polymerized acrylic and bis-acryl composite resins; blanks polymerized industrially and milled; and photopolymer resins built by additive manufacturing [1]. Mechanical properties differ among them. Milled PMMA polymers and printed resins have been compared with conventional materials for flexural strength and hardness [14, 15], and systematic reviews conclude that printed provisional resins are generally comparable or superior to conventional ones in several properties, with less wear volume loss in the studies reviewed [16, 17].
Wear has been measured after chewing simulation. In one study, printed and milled interim resins lost less volume than a conventional interim resin after 60,000 cycles, and mean surface roughness after wear was 0.59, 1.27, and 1.64 micrometers for printed, milled, and conventional materials [18]. A later study found no significant difference in wear volume or depth among conventional, milled, and two printed resins [19]. Wear of printed resin depends on build angle and post-polymerization, and specimens that were not post-polymerized wore significantly more [20]. In two-body tests, PEEK lost less material than PMMA or resin composite under lateral loading, and lateral loading produced more wear than axial loading [21]. In a three-body test with a pumice slurry over 120,000 cycles, mean volume loss was 0.08 mm³ for a composite, 0.23 mm³ for PEEK, and 0.55 mm³ for PMMA [22].
Wear simulation has known weaknesses. Simulators differ in the wear mechanisms they reproduce, and correlation with clinical wear has not been systematically established [23, 24]. A technical specification gives guidance on two- and three-body wear testing [25]. For the present purpose the key point is that every study cited above reported how much material was lost and none, as far as the abstracts show, examined the debris.
Particles from dental polymers
Direct evidence on particles from dental polymers is sparse and comes mainly from grinding. Dust produced by grinding dental prostheses of several materials differed in morphology, size, and composition and induced varying cytotoxicity in a macrophage cell line [26]. Nanoparticles can be released as by-products of milling and grinding, and a scientific update concluded that the main concern is inhalation exposure of laboratory and clinical personnel [27]. Chen and colleagues simulated wear and cleaning of dentures and grinding of resin-based materials: dentures released microplastic particles into artificial saliva during soaking and cleaning; grinding produced particles that settled in the clinic; and grinding-generated particles were toxic to oral keratinocytes and triggered inflammation in macrophages at concentrations the authors considered clinically encounterable [28]. The abstract does not state the quantities released from dentures. This study is the closest prior work identified. It concerns removable dentures and grinding, not functional wear of fixed provisional prostheses, and it must be read in full before the gap asserted here can be considered confirmed.
In orthodontics, clear aligners subjected to mechanical friction in artificial saliva for seven days shed microplastic particles, most between 5 and 20 micrometers [29], and commentaries have raised the matter as a clinical concern [30].
Chemical release
Resin-based materials also release soluble components. A meta-analysis found that quantities of eluted monomers vary widely with analytical conditions [31]. Acrylic resins are considered cytotoxic in vitro largely on account of leachable residual monomer [32], and eluates of a conventional PMMA reduced viability of human gingival fibroblasts more than those of a bis-acryl composite [33]. Particles have a high surface area and could act as carriers that release such components locally. A study of particles must therefore separate the effect of the particle from the effect of what dissolves from it.
Cellular response to polymer particles
The biology of polymer wear debris has been worked out in orthopedics. Macrophages phagocytose particles and release tumor necrosis factor and interleukins; the response depends on size, number, and volume [5, 8]. PMMA cement particles small enough to be phagocytosed induced tumor necrosis factor release from macrophages, whereas larger particles did not [7]. In a murine air-pouch model, PMMA and polyethylene particles provoked inflammatory responses [34]. Scavenger and Toll-like receptors participate in recognition of PMMA particles [35]. The immune response to polymer particles is regarded as non-specific and macrophage-mediated [6].
These findings come from a closed joint space in which particles accumulate for years. The mouth is an open system flushed by saliva. Extrapolation is not warranted without evidence that particles are retained in oral tissue. The literature on titanium particles around dental implants shows how hard it is to proceed from the presence of particles to a causal role in disease [36].
Terminology and methods for particle research
Plastic debris is categorized by size, with microplastics conventionally below 5 mm and nanoplastics defined variously as below 1 micrometer or below 100 nm [37, 38]. Health effects of ingested particles are uncertain, and data on intestinal uptake are scarce [39, 40]. Research on microplastics is prone to contamination from laboratory air, clothing, and plasticware, and reporting guidelines call for procedural blanks, recovery tests, and explicit detection limits [41]. For implant wear debris, an international standard describes isolation and characterization of polymer and metal particles [42], and in vitro cytotoxicity testing is standardized [43].
Summary
Provisional prosthesis materials wear measurably in simulators. Grinding of dental resins generates particles that affect cells in vitro. Polymer particles of phagocytosable size activate macrophages in other settings. What is missing is the middle of the chain: the particles produced by functional wear of provisional implant prostheses, their retention, and the response to them at relevant doses.
3. Research Gap
Table 1 sets out the chain from prosthesis to tissue effect and the status of each link as judged from the sources assessed.
| Link | Status | Basis |
|---|---|---|
| Provisional materials lose volume under simulated function | Established in vitro | Chewing-simulation studies [18, 19, 22] |
| Provisional prostheses wear and fracture in patients | Established clinically for fracture; wear not quantified in the sources found | Cohort data [3] |
| Lost volume is released as particles of defined number and size | Not characterized | No study identified |
| Dental resin particles from grinding affect cells in vitro | Supported in vitro | [26, 28] |
| Wear particles are retained at peri-implant tissue | Hypothetical | No data identified |
| Retained particles are taken up by tissue macrophages | Hypothetical in this setting; established in orthopedics | [5, 6] |
| Uptake alters soft-tissue healing or osseointegration | Hypothetical | No data identified |
| Clinical harm from provisional prosthesis wear | Not shown | No data identified |
The gap addressed here is the third row, with a first step toward the fourth under better-defined conditions. PubMed searches combining interim or provisional prostheses with wear particles, debris, and microplastics returned wear-volume studies and reviews of microplastics in dentistry and no characterization of wear debris from these prostheses. One three-body wear study measured roughness and volume without analyzing particles [22]. The absence of a matching record is weak evidence of absence: materials science journals outside PubMed and environmental science journals were not searched systematically.
4. Research Objective and Central Hypothesis
The objective is to characterize particles generated from provisional full-arch prosthesis materials by simulated function and handling and to measure the response of oral and immune cells to them.
Specific aims are:
- To generate wear debris from representative conventional, milled, and printed materials under two-body and three-body chewing simulation, toothbrush abrasion, and chairside adjustment, in a closed system with contamination control.
- To determine number, size distribution, shape, and chemical identity of the particles and to close the mass balance against measured volume loss.
- To determine the effect of environmental aging and of post-polymerization on particle generation.
- To measure responses of macrophages, gingival fibroblasts, oral keratinocytes, and osteoblasts to characterized, endotoxin-tested particles, alone and with bacterial co-stimulation, at doses bracketing an estimated local exposure.
- To test in an exploratory study whether wear of provisional prostheses in service can be quantified from scans at delivery and retrieval.
The central hypothesis is that materials and manufacturing routes with similar wear volume differ substantially in the number and size distribution of particles shed, and that the fraction between 0.3 and 10 micrometers determines macrophage response. The hypothesis would be refuted if size distributions were indistinguishable among materials, or if macrophage response tracked total mass irrespective of size.
A competing hypothesis deserves equal standing: that particles from functional wear are few, predominantly large, and biologically inconsequential at any plausible dose. The protocol is designed to be capable of supporting that conclusion, and such a result would be worth reporting.
5. Scientific and Theoretical Framework
From wear volume to particle number
Wear studies report volume. Biological response depends on number and surface area in particular size ranges. If a volume V is released as particles of equivalent spherical diameter d, the number of particles is
N=6V/(πd^3) (1)
and their total surface area is
A=6V/d (2)
For a size distribution with number density n(d), volume is V=π/6∫n(d) d^3 dd, and the number in a biologically relevant window (d_1,d_2) is N_w=∫_d_1^d_2 n(d) dd. Because of the cubic dependence, a small volume fraction of fine particles can dominate the count. Volume loss alone therefore cannot rank materials by particle burden.
Wear mechanisms and particle size
Different mechanisms are expected to yield different debris. Abrasive wear by hard asperities or third bodies cuts chips whose size scales with the abrasive. Adhesive and fatigue wear detach flakes from a surface layer weakened by cyclic contact. Fracture releases fragments visible to the eye. Printed resins are built in layers, and wear depends on build orientation [20], which suggests that interlayer boundaries may influence how fragments detach. Filled resins release filler particles together with matrix. Incompletely polymerized material wears faster [20] and may shed softer, smaller debris. Each of these statements is a mechanistic expectation to be tested by the characterization in Aim 2.
For sliding wear, volume is commonly described by the Archard relation,
V=K (F s)/H (3)
with load F, sliding distance s, hardness H, and a dimensionless coefficient K that carries the dependence on mechanism. The relation is used here only to organize how simulator results would be scaled to clinical loading. It says nothing about particle size.
Exposure chain
Let G be the rate of particle generation in a size window, in particles per day. A fraction φ is deposited at a tissue site of interest, and deposited particles are cleared with first-order rate λ. The local burden B obeys
dB/dt=φ G−λ B, B_∞=(φ G)/λ (4)
The generation rate can be measured in the laboratory. The deposited fraction and the clearance rate are unknown for any oral site. Equation (4) makes plain that a conclusion about tissue dose requires both, and that the laboratory study proposed here can bound only the first term. The in vitro dose range is accordingly chosen to span several orders of magnitude and is reported as particles and surface area per cell so that it can be reinterpreted when retention data become available.
Particle versus leachate
A cell exposed to polymer particles is also exposed to substances that dissolve from them. To separate the two, each particle preparation is tested alongside its own filtrate, obtained by incubating the particles in medium and removing them by ultrafiltration, and alongside particles that have been pre-extracted. A response to particles that is absent with filtrate and persists after extraction is attributed to the particle.
6. Methodology
Materials and specimens
Six material conditions are proposed: a conventional auto-polymerized PMMA of the kind used for denture conversion; a bis-acryl composite; an industrially polymerized PMMA blank, milled; two printed resins of different chemistry indicated for interim prostheses, printed and post-processed according to the manufacturers’ instructions; and one of the printed resins with post-polymerization deliberately omitted, as a worst case. Specimens are flat discs for standardized testing and anatomic molar segments for a subset. Surface finish follows a defined clinical polishing protocol. Half of the specimens are aged by water storage and thermal cycling before testing.
Particle generation
Chewing simulation is performed in sealed chambers of glass and stainless steel filled with filtered artificial saliva. Antagonists are enamel, zirconia, and the same polymer, representing natural teeth, a definitive opposing prosthesis, and an opposing provisional. Two-body tests use axial load with lateral sliding, in view of the larger wear reported under lateral loading [21]. Three-body tests add a food-simulating slurry; because an abrasive slurry contributes its own particles, three-body debris is analyzed with spectroscopic identification of every counted particle class. Loads and cycle numbers are selected with reference to published methods [23, 25]. No equivalence between cycles and months of clinical service is claimed, since such equivalences lack validation [24]; instead, simulator runs are matched to clinical wear depth if Stage 5 provides it.
Toothbrush abrasion is performed with a reciprocating brushing machine and a dentifrice slurry, and separately with water alone. Chairside adjustment is simulated by trimming specimens with burs of the kinds used clinically inside an enclosure from which airborne and settled particles are collected; this arm connects with earlier work on grinding dust [26, 28]. Fracture surfaces from specimens broken in bending are rinsed and the rinse analyzed for fragments.
Contamination control
All work with open samples is carried out in a laminar-flow cabinet. Plastic labware is avoided or, where unavoidable, is of a polymer spectroscopically distinguishable from the test materials. Liquids are filtered before use. Operators wear cotton laboratory coats. Procedural blanks, in which chambers are run without a polymer specimen, accompany every batch. Recovery is determined by spiking blanks with reference particles of known number. Counts are reported with blank subtraction and with limits of detection, in line with reporting guidelines [41].
Characterization
The volume lost from each specimen is measured by superimposing surface scans taken before and after testing. The entire chamber fluid is passed through a cascade of filters with decreasing pore size, and the final filtrate is retained for analysis of the submicrometer fraction. Filters are weighed on a microbalance after drying.
Particles on filters are imaged by scanning electron microscopy, and size and shape descriptors are obtained by image analysis with reference to the standard for wear particles [42]. Particles above about one micrometer are identified individually by infrared or Raman microspectroscopy. The submicrometer fraction is sized by a light-scattering method and its polymer mass determined by pyrolysis gas chromatography–mass spectrometry. Inorganic filler is identified by energy-dispersive spectroscopy. Residual monomer and other leachables in the fluid are quantified by chromatography.
The mass balance compares mass lost, calculated from volume loss and density, with the sum of particle mass on filters, polymer mass in the filtrate, and dissolved organics. A recovery well below unity would indicate loss of particles to chamber walls or a fraction too fine to capture, and would qualify all counts.
Particles for biological testing
Particles are pooled by material and condition, sterilized by a method shown not to alter size distribution, and tested for endotoxin, because endotoxin adsorbed to particles is a known source of spurious inflammatory responses. Dispersion in culture medium is verified by microscopy, since agglomeration changes the effective size that cells encounter. Size-fractionated preparations are produced by filtration to isolate the 0.3 to 10 micrometer window from larger and smaller fractions. Reference particles include a characterized polyethylene or polystyrene preparation and titanium particles.
Cell exposure
Human monocyte-derived macrophages are the primary cell type, with a monocytic cell line for screening. Human gingival fibroblasts, oral keratinocytes, and osteoblasts are tested in parallel. Doses are specified as particles per cell and as particle surface area per cell, across at least four orders of magnitude. Each condition is run with and without a low concentration of bacterial lipopolysaccharide, since oral tissues are continuously exposed to bacterial products and particle effects in orthopedic models are modified by such co-stimulation. Controls are the filtrate and pre-extracted particles described in Section 5.4.
Outcomes are viability by a standardized method [43]; release of tumor necrosis factor, interleukin-1β, and interleukin-6; reactive oxygen species; and particle uptake by confocal or electron microscopy. For osteoblasts, alkaline phosphatase activity and mineralization are added. Experiments use cells from at least three donors, with technical replicates, and are analyzed by mixed models with donor as a random effect.
Exploratory clinical stage
Provisional full-arch prostheses are scanned at delivery as part of the digital workflow. At conversion to the definitive prosthesis, with consent, the retrieved provisional is scanned again and the two scans are superimposed on unworn reference surfaces to estimate volume loss in service. Deposits on the intaglio surface are collected with particle-free instruments and examined spectroscopically for particles of the prosthesis polymer, with field blanks. The stage is descriptive. It estimates how much material a provisional loses in service and tests whether prosthesis-derived particles can be found near the tissue at all. It does not assess tissue response, and no biopsy is proposed.
Sample size and analysis
For particle generation, six specimens per material and condition is the planning figure, consistent with common practice in wear testing, to be revised after a pilot provides the variance of particle counts, which is expected to exceed that of wear volume. Size distributions are compared by their fractions in prespecified windows. The primary comparison is the number of particles between 0.3 and 10 micrometers per unit volume lost, across materials. For cell experiments, dose–response curves are fitted and compared among size fractions and materials. Multiplicity is controlled within each family of comparisons.
Ethics and safety
Laboratory stages involve commercially sourced cells or cells from donors under existing approvals. The clinical stage requires institutional review board approval and consent for use of retrieved prostheses and scan data. Laboratory personnel are protected against inhalation of grinding dust by enclosure and extraction [27]. No approval has been sought and no experiment has been performed.
7. Analytical Development
The indeterminacy of particle number
Take the mean volume loss reported for PMMA in the three-body study cited above, 0.55 mm³ after 120,000 cycles on a disc specimen [22]. Table 2 applies equations (1) and (2) on the assumption that this volume was released as spheres of a single diameter.
| Assumed diameter (µm) | Number of particles | Total surface area (cm²) |
|---|---|---|
| 100 | 1.1 × 10³ | 0.33 |
| 10 | 1.1 × 10⁶ | 3.3 |
| 1 | 1.1 × 10⁹ | 33 |
| 0.1 | 1.1 × 10¹² | 330 |
The same wear volume corresponds to about a thousand particles or about a trillion, depending on a quantity that no wear study of these materials has reported. The biologically active window identified for polyethylene, 0.3 to 10 micrometers [8], lies in the middle of this range. A material with twice the wear volume but coarse debris could deliver far fewer particles in that window than a material that wears less and sheds fine debris. The ranking of materials by wear volume [17, 18] therefore carries no information about their ranking by particle burden. This is the quantitative core of the argument for the protocol.
Mass and detectability
At a nominal density of about 1.18 g/cm³ for PMMA, 0.55 mm³ corresponds to about 0.65 mg. That mass is measurable on a microbalance, but only if the debris is collected quantitatively. Spread over a filter cascade and diluted by slurry in three-body tests, it approaches the limits of gravimetry, which is why the protocol relies on chemical quantification of polymer mass for the mass balance. In a two-body test with lower wear, the mass may be an order of magnitude smaller. Procedural blanks must then be very clean for the counts to be meaningful.
Dose scaling for cell experiments
Orthopedic studies report macrophage responses at particle volumes or numbers per cell that were set by experimental convenience. For the present protocol, doses are anchored to equation (4) in a deliberately crude way. The generation rate G in the active window is measured per cycle in the simulator and scaled to daily function under stated assumptions about chewing cycles and load. The product φ/λ, the ratio of deposited fraction to clearance rate, is unknown and is treated as a free parameter. The dose range is chosen so that it covers the burden predicted for values of that ratio across several orders of magnitude. If no cellular response appears even at the upper end, where nearly all generated particles would have to be retained for days, the competing hypothesis of biological insignificance is supported. If a response appears only at such doses, the conclusion is the same. Only a response at doses reachable with small retained fractions would justify proceeding to retention studies.
What the laboratory study cannot show
No in vitro experiment establishes that particles reach or remain in tissue, that macrophages in mucosa behave as cultured cells do, or that any response affects healing. The protocol can show whether the necessary first conditions are met: that particles of relevant size are produced in relevant numbers, and that cells respond to them at doses that are not absurd.
8. Discussion
The proposal sits between two bodies of work that have not been connected. Dental materials research measures the wear of provisional polymers with care and stops at the specimen surface. Particle toxicology has a mature account of how macrophages respond to polymer debris and has had no reason to look at provisional prostheses. The missing piece is descriptive and, in principle, simple to supply.
Several features of the clinical setting make the question more than academic. A provisional full-arch prosthesis is in place during wound healing and osseointegration, when tissues are most open to foreign material. It lies directly over the implant sites. It is made of the least wear-resistant materials used in fixed prosthodontics, and newer printed resins vary in chemistry and in degree of conversion according to how they are processed [20]. Surgical conversion of a denture involves grinding acrylic at the chairside, and grinding is the one mode of particle generation for which cellular effects have been reported [26, 28].
There are equally good reasons for restraint. The mouth is not a joint capsule. Saliva clears particles continuously, and the gut receives them along with a diet that contains other particulates. PMMA has been used in the mouth for the better part of a century in removable dentures, which present a far larger wearing surface for far longer, without a recognized syndrome of particle disease. The clinical record of provisional full-arch prostheses is dominated by fracture, not by unexplained tissue reactions [3]. The prior probability that wear particles from provisionals have a clinically important effect on peri-implant healing is, on this reasoning, low. The value of the study lies partly in replacing that judgment with data, and partly in establishing methods and baseline values that will be needed as printed resins of new composition enter use.
How the result is communicated matters. Research on microplastics attracts attention, and detection of particles is easily reported as evidence of harm. Detection is not harm. The associations reported between tissue microplastics and disease are observational [11], and reviews of the dental literature stress the weakness of exposure data [12]. A study that found measurable particle release from provisional prostheses and no cellular response at realistic doses should say exactly that.
The design choices that most affect credibility are contamination control and the mass balance. Without clean blanks, counts of small particles are uninterpretable. Without a mass balance, a low count cannot be distinguished from a failure to capture. The decision to test particles against their own filtrates addresses a confusion that runs through the literature on resin cytotoxicity, where effects of leachable monomer [31, 32] and effects of particles are seldom separated.
9. Clinical Significance
No change in clinical practice follows from this proposal. If the laboratory work showed that some materials or processing conditions shed many more fine particles than others, that information would bear on material selection and on the importance of complete post-polymerization, alongside strength and cost. If chairside grinding proved to be the dominant source, simple measures such as extraoral adjustment, suction, and rinsing before reinsertion would be indicated on precautionary grounds, and these are already good practice. If particle release proved negligible, a speculative concern could be set aside. Patients should not be told that provisional prostheses release harmful microplastics; nothing in the evidence supports such a statement.
10. Limitations
Simulators reproduce clinical wear imperfectly, and debris generated in a chamber may differ from debris generated in the mouth. Particles may agglomerate or adhere to surfaces and be undercounted. Methods for nanoplastics are less reliable than those for larger particles, and the finest fraction may be characterized only by mass. Sterilization and handling may alter particles before they reach cells. Cultured cells exposed for hours to days do not represent tissue exposed intermittently for months. The retention and clearance terms of the exposure chain are not addressed experimentally. The closest prior study was assessed only from its abstract and may contain data that narrow the gap. The density used in Section 7.2 is a nominal handbook value and was not taken from a verified source in this project. The literature search was confined to PubMed and a registry and did not cover materials science or environmental databases.
11. Future Validation
The first step is a pilot that establishes blank levels, recovery, and the feasibility of the mass balance for one material. The full generation and characterization study follows. Cell experiments proceed only with characterized, endotoxin-tested particles. If a response is found at doses compatible with modest retention, the next questions are retention itself, for which an explanted mucosal model or analysis of tissue removed for clinical reasons would be needed, and the comparison with definitive materials. An interlaboratory comparison of particle counts would be required before any values were used for material ranking or standards.
12. Conclusion
Provisional full-arch implant prostheses wear, and the particles they shed have not been characterized. Published wear volumes are compatible with particle numbers that differ by nine orders of magnitude, depending on a size distribution that is unknown. A laboratory protocol is described that would generate, isolate, and characterize these particles under contamination control and test the response of oral and immune cells at doses tied to an explicit exposure model. The possibility that the particles are biologically unimportant is treated as a live hypothesis. No experiment has been performed, and no clinical effect is claimed.
Cite this paper
Jain S, Gupta A. Wear-Generated Polymer Particles From Provisional Full-Arch Implant Prostheses: A Laboratory Protocol for Particle Generation, Characterization, and Assessment of Cellular Response. Working paper. Center for Implant Dentistry; 2026. Available from: https://bayareaimplantdentistry.com/clinician-research-and-publications/polymer-wear-particles-provisional-prostheses
References
- Revilla-León M, Özcan M. Additive Manufacturing Technologies Used for Processing Polymers: Current Status and Potential Application in Prosthetic Dentistry. J Prosthodont. 2019;28(2):146-158. doi:10.1111/jopr.12801 (opens in a new tab). PMID: 29682823 (opens in a new tab).
- Bender J, Piermatti J, Feit D, Minhas T. Influence of material and technique of conversion on interim prosthesis fracture. J Prosthodont. 2025;34(9):947-955. doi:10.1111/jopr.70020 (opens in a new tab). PMID: 40897985 (opens in a new tab).
- Mendonça C, de Macedo D, Nicolai C, Madeira H, Van Dooren E, Norré D, et al. Digital Full-Arch Implant-Supported Polymethyl Methacrylate Interim Prosthesis: A Practice-Based Cohort Study on Survival and Quality of Life. Int J Prosthodont. 2024;37(4):394-403. doi:10.11607/ijp.8468 (opens in a new tab). PMID: 37824125 (opens in a new tab).
- Papaspyridakos P, Chen CJ, Chuang SK, Weber HP, Gallucci GO. A systematic review of biologic and technical complications with fixed implant rehabilitations for edentulous patients. Int J Oral Maxillofac Implants. 2012;27(1):102-10. PMID: 22299086 (opens in a new tab).
- Ingham E, Fisher J. The role of macrophages in osteolysis of total joint replacement. Biomaterials. 2005;26(11):1271-86. doi:10.1016/j.biomaterials.2004.04.035 (opens in a new tab). PMID: 15475057 (opens in a new tab).
- Goodman SB. Wear particles, periprosthetic osteolysis and the immune system. Biomaterials. 2007;28(34):5044-8. doi:10.1016/j.biomaterials.2007.06.035 (opens in a new tab). PMID: 17645943 (opens in a new tab).
- Horowitz SM, Doty SB, Lane JM, Burstein AH. Studies of the mechanism by which the mechanical failure of polymethylmethacrylate leads to bone resorption. J Bone Joint Surg Am. 1993;75(6):802-13. doi:10.2106/00004623-199306000-00002 (opens in a new tab). PMID: 8314821 (opens in a new tab).
- Green TR, Fisher J, Stone M, Wroblewski BM, Ingham E. Polyethylene particles of a ‘critical size’ are necessary for the induction of cytokines by macrophages in vitro. Biomaterials. 1998;19(24):2297-302. doi:10.1016/s0142-9612(98)00140-9 (opens in a new tab). PMID: 9884043 (opens in a new tab).
- Leslie HA, van Velzen MJM, Brandsma SH, Vethaak AD, Garcia-Vallejo JJ, Lamoree MH. Discovery and quantification of plastic particle pollution in human blood. Environ Int. 2022;163:107199. doi:10.1016/j.envint.2022.107199 (opens in a new tab). PMID: 35367073 (opens in a new tab).
- Ragusa A, Svelato A, Santacroce C, Catalano P, Notarstefano V, Carnevali O, et al. Plasticenta: First evidence of microplastics in human placenta. Environ Int. 2021;146:106274. doi:10.1016/j.envint.2020.106274 (opens in a new tab). PMID: 33395930 (opens in a new tab).
- Marfella R, Prattichizzo F, Sardu C, Fulgenzi G, Graciotti L, Spadoni T, et al. Microplastics and Nanoplastics in Atheromas and Cardiovascular Events. N Engl J Med. 2024;390(10):900-910. doi:10.1056/NEJMoa2309822 (opens in a new tab). PMID: 38446676 (opens in a new tab).
- Šimunović L, Bačić I, Meštrović S. Micro- and Nanoplastics in Dentistry: Challenges in Obtaining High-Quality Evidence. Materials (Basel). 2025;18(18). doi:10.3390/ma18184269 (opens in a new tab). PMID: 41010113 (opens in a new tab).
- Umrai Shariff K, Le A, Goodwin-Loughton E, Chung M, Ali A, Farella M, et al. Microplastics and nanoplastics in clinical dentistry and orthodontics: leaching, health implications, and future directions: a narrative review. Prog Orthod. 2025;26(1):49. doi:10.1186/s40510-025-00597-9 (opens in a new tab). PMID: 41296116 (opens in a new tab).
- Digholkar S, Madhav VN, Palaskar J. Evaluation of the flexural strength and microhardness of provisional crown and bridge materials fabricated by different methods. J Indian Prosthodont Soc. 2016;16(4):328-334. doi:10.4103/0972-4052.191288 (opens in a new tab). PMID: 27746595 (opens in a new tab).
- Alp G, Murat S, Yilmaz B. Comparison of Flexural Strength of Different CAD/CAM PMMA-Based Polymers. J Prosthodont. 2019;28(2):e491-e495. doi:10.1111/jopr.12755 (opens in a new tab). PMID: 29377319 (opens in a new tab).
- Jain S, Sayed ME, Shetty M, Alqahtani SM, Al Wadei MHD, Gupta SG, et al. Physical and Mechanical Properties of 3D-Printed Provisional Crowns and Fixed Dental Prosthesis Resins Compared to CAD/CAM Milled and Conventional Provisional Resins: A Systematic Review and Meta-Analysis. Polymers (Basel). 2022;14(13). doi:10.3390/polym14132691 (opens in a new tab). PMID: 35808735 (opens in a new tab).
- Alzahrani SJ, Hajjaj MS, Azhari AA, Ahmed WM, Yeslam HE, Carvalho RM. Mechanical Properties of Three-Dimensional Printed Provisional Resin Materials for Crown and Fixed Dental Prosthesis: A Systematic Review. Bioengineering (Basel). 2023;10(6). doi:10.3390/bioengineering10060663 (opens in a new tab). PMID: 37370594 (opens in a new tab).
- Myagmar G, Lee JH, Ahn JS, Yeo IL, Yoon HI, Han JS. Wear of 3D printed and CAD/CAM milled interim resin materials after chewing simulation. J Adv Prosthodont. 2021;13(3):144-151. doi:10.4047/jap.2021.13.3.144 (opens in a new tab). PMID: 34234924 (opens in a new tab).
- Çiçek Y, Küçük C. Wear of interim resin materials manufactured by 3D printing and CAD/CAM milling following chewing simulation. BMC Oral Health. 2025;25(1):1679. doi:10.1186/s12903-025-07105-9 (opens in a new tab). PMID: 41146159 (opens in a new tab).
- Wan Q, Lee JH, Daher R, Karasan D, Myagmar G, Sailer I. Wear Resistance of Additively Manufactured Resin with Different Printing Parameters and Postpolymerization Conditions. Int J Prosthodont. 2024;37(7):55-62. doi:10.11607/ijp.8538 (opens in a new tab). PMID: 38489221 (opens in a new tab).
- Wimmer T, Huffmann AM, Eichberger M, Schmidlin PR, Stawarczyk B. Two-body wear rate of PEEK, CAD/CAM resin composite and PMMA: Effect of specimen geometries, antagonist materials and test set-up configuration. Dent Mater. 2016;32(6):e127-36. doi:10.1016/j.dental.2016.03.005 (opens in a new tab). PMID: 27033460 (opens in a new tab).
- Elsadany AF, Borg HS, Elshenawy EA. Effect of three-body wear on the surface properties of different polymer-based CAD/CAM dental restorative and prosthetic materials. BMC Oral Health. 2026;26(1). doi:10.1186/s12903-026-09028-5 (opens in a new tab). PMID: 42399941 (opens in a new tab).
- Lambrechts P, Debels E, Van Landuyt K, Peumans M, Van Meerbeek B. How to simulate wear? Overview of existing methods. Dent Mater. 2006;22(8):693-701. doi:10.1016/j.dental.2006.02.004 (opens in a new tab). PMID: 16712913 (opens in a new tab).
- Heintze SD. How to qualify and validate wear simulation devices and methods. Dent Mater. 2006;22(8):712-34. doi:10.1016/j.dental.2006.02.002 (opens in a new tab). PMID: 16574212 (opens in a new tab).
- International Organization for Standardization. ISO/TS 14569-2:2001. Dental materials—Guidance on testing of wear—Part 2: Wear by two- and/or three-body contact. Geneva: ISO; 2001.
- Wang W, Li T, Luo X, Zhang K, Cao N, Liu K, et al. Cytotoxic effects of dental prosthesis grinding dust on RAW264.7 cells. Sci Rep. 2020;10(1):14364. doi:10.1038/s41598-020-71485-x (opens in a new tab). PMID: 32873894 (opens in a new tab).
- Schmalz G, Hickel R, van Landuyt KL, Reichl FX. Scientific update on nanoparticles in dentistry. Int Dent J. 2018;68(5):299-305. doi:10.1111/idj.12394 (opens in a new tab). PMID: 29786135 (opens in a new tab).
- Chen Y, Chen J, Guo J, Yao M, Liu Y, Qian J, et al. Release of microplastics during dental procedures and denture wear: Impact on dental personnel and patients. J Hazard Mater. 2025;494:138463. doi:10.1016/j.jhazmat.2025.138463 (opens in a new tab). PMID: 40319856 (opens in a new tab).
- Quinzi V, Orilisi G, Vitiello F, Notarstefano V, Marzo G, Orsini G. A spectroscopic study on orthodontic aligners: First evidence of secondary microplastic detachment after seven days of artificial saliva exposure. Sci Total Environ. 2023;866:161356. doi:10.1016/j.scitotenv.2022.161356 (opens in a new tab). PMID: 36603638 (opens in a new tab).
- Krishnan V. Microplastics: An orthodontic concern!. J World Fed Orthod. 2024;13(3):103-104. doi:10.1016/j.ejwf.2024.05.001 (opens in a new tab). PMID: 38830718 (opens in a new tab).
- Van Landuyt KL, Nawrot T, Geebelen B, De Munck J, Snauwaert J, Yoshihara K, et al. How much do resin-based dental materials release? A meta-analytical approach. Dent Mater. 2011;27(8):723-47. doi:10.1016/j.dental.2011.05.001 (opens in a new tab). PMID: 21664675 (opens in a new tab).
- Gautam R, Singh RD, Sharma VP, Siddhartha R, Chand P, Kumar R. Biocompatibility of polymethylmethacrylate resins used in dentistry. J Biomed Mater Res B Appl Biomater. 2012;100(5):1444-50. doi:10.1002/jbm.b.32673 (opens in a new tab). PMID: 22454327 (opens in a new tab).
- Della Rocca Y, Traini EM, Trubiani O, Traini T, Mazzone A, Marconi GD, et al. Biological Effects of PMMA and Composite Resins on Human Gingival Fibroblasts: An In Vitro Comparative Study. Int J Mol Sci. 2024;25(9). doi:10.3390/ijms25094880 (opens in a new tab). PMID: 38732100 (opens in a new tab).
- Wooley PH, Morren R, Andary J, Sud S, Yang SY, Mayton L, et al. Inflammatory responses to orthopaedic biomaterials in the murine air pouch. Biomaterials. 2002;23(2):517-26. doi:10.1016/s0142-9612(01)00134-x (opens in a new tab). PMID: 11761173 (opens in a new tab).
- Yamada C, Beron-Pelusso C, Algazzaz N, Heidari A, Luz D, Rawas-Qalaji M, et al. Age-dependent effect between MARCO and TLR4 on PMMA particle phagocytosis by macrophages. J Cell Mol Med. 2019;23(8):5827-5831. doi:10.1111/jcmm.14494 (opens in a new tab). PMID: 31225947 (opens in a new tab).
- Mombelli A, Hashim D, Cionca N. What is the impact of titanium particles and biocorrosion on implant survival and complications? A critical review. Clin Oral Implants Res. 2018;29 Suppl 18:37-53. doi:10.1111/clr.13305 (opens in a new tab). PMID: 30306693 (opens in a new tab).
- Hartmann NB, Hüffer T, Thompson RC, Hassellöv M, Verschoor A, Daugaard AE, et al. Are We Speaking the Same Language? Recommendations for a Definition and Categorization Framework for Plastic Debris. Environ Sci Technol. 2019;53(3):1039-1047. doi:10.1021/acs.est.8b05297 (opens in a new tab). PMID: 30608663 (opens in a new tab).
- Gigault J, Halle AT, Baudrimont M, Pascal PY, Gauffre F, Phi TL, et al. Current opinion: What is a nanoplastic?. Environ Pollut. 2018;235:1030-1034. doi:10.1016/j.envpol.2018.01.024 (opens in a new tab). PMID: 29370948 (opens in a new tab).
- Wright SL, Kelly FJ. Plastic and Human Health: A Micro Issue?. Environ Sci Technol. 2017;51(12):6634-6647. doi:10.1021/acs.est.7b00423 (opens in a new tab). PMID: 28531345 (opens in a new tab).
- Stock V, Böhmert L, Lisicki E, Block R, Cara-Carmona J, Pack LK, et al. Uptake and effects of orally ingested polystyrene microplastic particles in vitro and in vivo. Arch Toxicol. 2019;93(7):1817-1833. doi:10.1007/s00204-019-02478-7 (opens in a new tab). PMID: 31139862 (opens in a new tab).
- Cowger W, Booth AM, Hamilton BM, Thaysen C, Primpke S, Munno K, et al. Reporting Guidelines to Increase the Reproducibility and Comparability of Research on Microplastics. Appl Spectrosc. 2020;74(9):1066-1077. doi:10.1177/0003702820930292 (opens in a new tab). PMID: 32394727 (opens in a new tab).
- International Organization for Standardization. ISO 17853:2011. Wear of implant materials—Polymer and metal wear particles—Isolation and characterization. Geneva: ISO; 2011.
- International Organization for Standardization. ISO 10993-5:2009. Biological evaluation of medical devices—Part 5: Tests for in vitro cytotoxicity. Geneva: ISO; 2009.